Tip of the Day 79: Looking for Change

Tip # 78 explains trends and cycles in terms of stability. This leads to the next concept: A stable process can change and it is important to notice it and understand it.

Below is an example showing 24 hours of data with a variety of different events. Typical events seen in summary data include:

  • Drop-outs or spikes: Usually caused by cycle stops with re-stabilization but sometimes just a random event or randomly blocked gates. The Sequence Time / Cycle Time always shows a spike
  • Trends downward or upward in an otherwise stable process
  • Sudden steps up or down in a summary value.

Each of these are indicators of something changing and therefore the parts will be different in some way.


Short Course in Graph Interpretation

  • Flat(ish) Line:

    At the start of this period the process is stable: no cyclical shapes or trends appear the data.

  • Spikes:

    Occasionally there is a spike on cavity # 7 integral. These are not uncommon in injection molding are the reason for using in-cavity measurement for containment.

  • Spikes in Cycle Time:

    Whenever a cycle stops a spike in the cycle time shows how long it was stopped.

  • Drop Outs:

    Then when the process starts several parts are produced that are out of specification. This is due to the mold cooling about 40°F and the a long residence time degrading the material. These can show up as drop-outs and sometimes as spikes.

    Drop outs are also caused by random events like stuck gates or unmelted pellets.

  • Downward Trend:

    In this example the material feed was changed to a new lot. For some reason the further the material feed got into the new lot the lower the viscosity. This caused the integrals to trend upwards – lower viscosity => easier to fill and pack.

  • Step in Data:

    A technician noticed the integrals crossing the alarm settings (cavity # 8) and the machine throwing parts away. Not understanding the material change he re-adjusted the process to bring the integrals back into line by lowering the hold pressure. This shows as a step in the Average Value / Stable Hold Pressure (brown curve).

    Generally steps indicate that an operator changed something. Occasionally a step occurs when something breaks (e.g. a core pin). When barrel heaters or mold temperature controls go awry you usually see a trend.

  • Notes:

    Notes are also part of the summary data. If technicians are careful to enter them they will help to interpret what happened at these various events.